Leave Your Message
Part Silver Causes and Improvement for Injection Molding
News

Part Silver Causes and Improvement for Injection Molding

2026-11-02
  • Material Factors
  1. Moisture absorption of raw material (Most common)

Hygroscopic materials (PC, PA, PET, PMMA, etc.) absorb moisture. Water vaporizes under high temperature and creates moisture splay.

Improvements:

- Dry strictly in accordance with material specifications: PC 120℃ / 3~4h; PA 80~85℃ / 4h; PMMA 80℃ / 3~4h

- Seal and keep warm after drying to avoid re-absorption of moisture; verify hot air, temperature and air volume of the hopper dryer

- Control regrind ratio. Regrind tends to absorb moisture and shall be dried separately in advance

 

  1. Thermal decomposition of material (Degradation splay)

Excessive barrel temperature or long residence time of material inside the screw causes plastic decomposition and releases low-molecular volatiles.

Improvements:

- Reduce barrel and nozzle temperature; do not exceed the upper limit recommended by material supplier

- Shorten melt residence time; lower temperature or purge the screw during machine stoppage

- Avoid excessive back pressure which leads to overheating by shear; reduce screw speed

 

  1. Raw material contamination, volatilization of additives / color masterbatch

Volatiles from color pigment, additives and release agent mix with melt and cause gas splay.

Improvements:

- Switch to low-volatility color masterbatch and additives; ensure release agent does not splash onto pellets

- Check if foreign materials are mixed into raw resin

 

  • Mold Factors
  1. Poor venting

Air trapped in cavity and gas generated by melt cannot escape, and are squeezed and stretched by molten plastic to form splay (often accompanied by burn marks).

Improvements:

- Add vent slots; vent depth shall match the material (0.02~0.03mm for PC generally). Place vents at melt end and weld line positions

- Check vent blockage and clean mold regularly; add venting via inserts or ejector pins

- Optimize gate location to prevent air trapping in thin-wall areas

 

  1. Improper gate / runner design

Undersized gate creates strong shear; high shear rate heats up melt rapidly and triggers material decomposition and gas generation. Too small runner brings high flow resistance.

Improvements:

- Enlarge gate appropriately to reduce shear rate; fan gate and side gate are preferred, avoid tiny pin gate

- Polish runners to reduce flow resistance

 

  1. Oil contamination on mold surface & excessive release agent

Over-sprayed release agent volatilizes under heat and enters cavity to form splay.

Improvements:

- Reduce release agent usage; prefer silicone-free release agent; wipe off oil stains on mold surface

 

  • Injection Molding Process Factors
  1. Excessively fast injection speed

High-speed injection leaves insufficient time for gas evacuation. Strong shear also easily causes material decomposition, and splay streaks elongate along flow direction.

Improvements:

- Multi-stage injection: low speed at gate section, speed up after filling the front cavity

- Reduce injection speed

 

  1. Improper back pressure and screw speed

High back pressure and fast screw rotation generate shear heat on melt and induce material decomposition & gas release.

Improvements:

- Reduce back pressure and screw speed moderately, as long as melt homogeneity is guaranteed

 

  1. Unreasonable injection pressure & packing pressure

Excessive pressure compresses trapped gas and aggravates splay appearance.

Improvements:

- Lower injection pressure; avoid early and excessive packing pressure

 

  1. Long melt residence time inside barrel

Long cycle time or small shot volume keeps resin staying at high temperature for a long time and leads to decomposition.

Improvements:

- Shorten residence time; increase shot cushion or purge the screw if necessary