Causes and Improvements for Sink Marks in Injection Molding
News

Causes and Improvements for Sink Marks in Injection Molding

2026-10-05

Volume shrinkage occurs when plastic cools and solidifies. Thickwall sections, ribs and boss positions generate substantial heat and cool slowly. The outer surface of the part cools first to form a hard shell, while the inner material continues to shrink and pulls the surface inward, resulting in depressions. Crystalline materials (PP, PA, POM) produce more obvious sink marks than amorphous materials (ABS, PC).

I. Product Structure Related Causes
 1.Uneven wall thickness and local material accumulation: Excessively thick ribs and bosses; sink marks are highly likely to form on the reverse side when rib thickness exceeds 60% of the main wall thickness; abrupt wallthickness changes without transition fillet radii.
  Improvements: Control rib thickness at 50% to 60% of the main wall thickness; implement boss coring / sink relief for bosses; remove material from thick-wall areas and adopt smooth transitions to avoid abrupt wall thickness variations.


II. Mold Related Causes
 1.Undersized gate or improper gate location An undersized gate freezes off prematurely, closing the packing feed path. When the gate is too far from thick-wall zones, pressure transmission decays and thick sections cannot get compensatory feeding.
  Improvements: Increase gate thickness; locate gates at thick-wall positions as much as possible; adopt high-flow gate types (fan gate, direct gate); enlarge runner cross section to delay gate freeze off.

 2.Poor cooling channel design No cooling channels for thick-wall sections or ribs; cooling channels are too far from the cavity; unbalanced cooling channels between core and cavity plates lead to asynchronous cooling and delayed solidification in local areas.
  Improvements: Add independent cooling channels for thick-wall zones; ensure balanced cooling on both cavity and core sides, and realize sequential solidification as far as possible: areas far from the gate cool first, and the gate area cools last for continuous compensatory feeding.


 3.Insufficient venting Trapped air in thick zones creates back pressure, hindering melt filling and packing feeding, which indirectly causes sink marks, often accompanied by internal vacuum voids.
  Improvements: Add vent slots at sinkmark positions to guarantee smooth venting.


 4.Unbalanced runners for multi-cavity mold Inconsistent melt feeding among cavities leads to insufficient packing pressure in individual cavities and triggers sink marks.
  Improvements: Balance runners and perform runner tuning to achieve uniform filling of all cavities.

III. Injection Molding Process Related Causes

  1. Insufficient packing pressure or too short packing time (most common) Packing is the core for compensatory shrinkage compensation. Insufficient packing time causes early gate freeze off so that compensatory feeding cannot continue.

Improvements: Increase packing pressure (normally 60 to 80% of injection pressure); extend packing time until part weight no longer increases (gate freeze off point); ensure sufficient screw cushion.

  1. Excessively high barrel temperature Higher melt temperature brings larger volume shrinkage during cooling.

Improvements: Lower barrel temperature appropriately.

  1. Excessively high mold temperature High mold temperature extends cooling cycle and increases shrinkage magnitude.

Improvements: Reduce mold temperature properly without compromising surface appearance; keep temperature difference between cavity and core below 10 °C.

  1. Improper injection speed Overfast filling leaves no time for air evacuation; over-slow filling causes premature solidification of melt front and poor pressure transmission.

Improvements: Adopt multi-stage injection and reduce speed for thick-wall regions to achieve stable filling.