Leave Your Message
Causes and Solutions for Air Bubble / Void Defect in Injection Molding
News

Causes and Solutions for Air Bubble / Void Defect in Injection Molding

2026-10-23
  • Material-Related Causes
  1. Raw material moisture absorption; water vaporizes under high temperature to form bubbles (highly hygroscopic materials: PC, PA, PET, PMMA are high-risk)

   - Solution: Strictly dry material following specified temperature & duration; install hopper dryer; check dryer dew point and hot air circulation; prevent re-absorption of moisture after drying.

  1. Thermal degradation of resin, generating decomposition gas (overheating, long residence time, high regrind ratio, degraded regrind)

   - Solution: Reduce barrel temperature and back pressure; shorten screw residence time; lower regrind percentage; check regrind for contamination; add stabilizer to avoid thermal decomposition.

  1. Volatiles in material, additive blooming or foreign contaminants

   - Solution: Change material batch; reduce lubricant / plasticizer dosage; clean barrel and hopper thoroughly.

 

  • Part & Mold Structural Causes (Priority for fixed-location defects)
  1. Thick wall sections create internal vacuum voids (thick stock, bosses, heavy ribs)

   - Solution: Reduce wall thickness, add volcano cut-out / core-out; maintain uniform wall thickness; smooth transition for thickness variation; evaluate gas-assisted injection molding if applicable.

  1. Poor venting, blocked vents or improperly located vents; melt front encapsulates gas inside cavity

   - Solution: Add vents at melt end / last fill position; control vent depth by material (0.015~0.02 mm for PC / PMMA); regularly clean carbon and oil deposits on vents; add parting line vents, insert vents or ejector pin vents.

  1. Improper runner / gate design: Undersized gate, gate far from thick sections, gas trapped due to filling sequence; overlong runner with high resistance

   - Solution: Enlarge gate or reposition gate to feed thick sections first; switch to fan gate / tab gate; shorten runner; check hot manifold for local overheating and stagnant degraded material.

  1. Unbalanced mold cooling: Rapid skin solidification seals surface before internal gas escapes or shrinkage forms vacuum voids

   - Solution: Optimize cooling channels; add water lines close to thick stock; uniform water distance; apply beryllium copper inserts for enhanced cooling on thick areas.

 

  • Injection Process Causes
  1. Excessive injection speed causes turbulent melt front and air entrapment

   - Solution: Multi-stage speed control; slow down speed at end of fill for stable venting.

  1. Insufficient packing pressure / short packing time: Not enough melt feed to compensate shrinkage in thick sections → vacuum voids

Note: Vacuum voids respond well to packing adjustment; trapped-air bubbles rarely improve with higher packing and may burn instead.

   - Solution: Increase packing pressure and extend packing time; set proper switch-over position; avoid excessive packing which induces stress and sticking.

  1. Low back pressure and fast screw speed entrain air during plasticization

   - Solution: Increase back pressure moderately, reduce screw speed for denser melt and air release; apply suck-back after metering to relieve barrel pressure.

  1. Overhigh barrel / nozzle temperature triggers material degradation and gas generation

   - Solution: Reduce barrel zone temperature especially front zone and nozzle; shorten cycle time to reduce melt residence time.

  1. Improper mold temperature: High mold temp leads to slow cooling, degradation and shrinkage voids; low mold temp causes early skin freeze-off and trapped gas

   - Solution: Set mold temperature per material specification: PC 80–110℃, PMMA 70–90℃ for reference.

  1. Insufficient injection pressure limits filling and prevents gas from moving toward vents

   - Solution: Raise injection pressure moderately with multi-speed profile.